CN102887672B - 一种以碎玻璃为基质的加气砖及其加工方法 - Google Patents

一种以碎玻璃为基质的加气砖及其加工方法 Download PDF

Info

Publication number
CN102887672B
CN102887672B CN201210320638.4A CN201210320638A CN102887672B CN 102887672 B CN102887672 B CN 102887672B CN 201210320638 A CN201210320638 A CN 201210320638A CN 102887672 B CN102887672 B CN 102887672B
Authority
CN
China
Prior art keywords
air
powder
parts
glass cullet
cullet
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201210320638.4A
Other languages
English (en)
Other versions
CN102887672A (zh
Inventor
张爱民
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
HAINAN GUANGSHENG NEW BUILDING MATERIALS CO., LTD.
Original Assignee
WUHE NEW ENVIRONMENTAL PROTECTION BUILDING MATERIALS FACTORY OF BENGBU AIMIN AUTOMOBILE SERVICE CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by WUHE NEW ENVIRONMENTAL PROTECTION BUILDING MATERIALS FACTORY OF BENGBU AIMIN AUTOMOBILE SERVICE CO Ltd filed Critical WUHE NEW ENVIRONMENTAL PROTECTION BUILDING MATERIALS FACTORY OF BENGBU AIMIN AUTOMOBILE SERVICE CO Ltd
Priority to CN201210320638.4A priority Critical patent/CN102887672B/zh
Publication of CN102887672A publication Critical patent/CN102887672A/zh
Application granted granted Critical
Publication of CN102887672B publication Critical patent/CN102887672B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种以碎玻璃为基质的加气砖及其加工方法,其组成原料的重量份为:碎玻璃40-55、城市污泥5-10、水泥5-8、云母粉5-10、膨胀珍珠岩14-16、石膏4-5、改性草木灰2-4、铝粉0.03-0.05、凹凸棒土0.5-1、平平加0.03-0.04、纯碱0.03-0.05、氢氧化铝0.01-0.02、三乙醇胺0.01-0.02和壳聚糖0.3-0.5。本发明通过采用碎玻璃和城市玻璃作为加气砖的成分,有效的减少了环境污染,变废为宝,保护了环境;减少了能源消耗;本发明加气砖隔热与隔音性能均好,较现有加气砖有明显提高;同时本发明通过优化配方用料,本发明的强度、抗冻性有了明显提高。

Description

一种以碎玻璃为基质的加气砖及其加工方法
技术领域
本发明涉及新型建材领域,具体属于一种以碎玻璃为基质的加气砖及其加工方法。
背景技术
加气砖是通过高温蒸压设备工艺生产的加气砖砌块,即采用包括蒸压在内的其他各种工艺生产的砖品,加气砖是一种新型的墙体建材,它的独特之处在于它是一种非常轻型的保温隔热的新型建筑墙材,而我国的该项技术开始的比较晚,比国外整整落后了四十年,但是,我国的加气砖行业的发展确实非常迅速的,现在国内的加气砖技术工艺水平已经可以达到了国际先进水平。 
加气砖最大优势就是节约土地资源,不用浪费大量的耕地,而且它的原料的来源非常的广泛,灰沙,矿渣,粉煤灰和煤矸石等等都是做加气砖的原材料,而且加气砖的性能特点非常的优越,有非常好的可加工能力和隔热和保温能力,而且可塑性非常的强,有非常好的加工特性,加气砖原料的研究和加工技术需要进一步的提高。
发明内容
本发明的目的在于提供一种以碎玻璃为基质的加气砖及其加工方法,碎玻璃用量大、节能环保,缓解碎玻璃堆存处理带来的环境污染问题,同时为加气砖提供了新的原料来源。
为了实现上述目的本发明采用如下技术方案:
以碎玻璃为基质的加气砖,其组成原料的重量份为:碎玻璃40-55、城市污泥5-10、水泥5-8、云母粉5-10、膨胀珍珠岩14-16、石膏4-5、改性草木灰2-4、铝粉0.03-0.05、凹凸棒土0.5-1、平平加0.03-0.04、纯碱0.03-0.05、氢氧化铝0.01-0.02、三乙醇胺0.01-0.02和壳聚糖0.3-0.5。
以碎玻璃为基质的加气砖的加工方法,包括以下步骤:
(1)原材料的处理:原材料包括碎玻璃、城市污泥、水泥、云母粉、膨胀珍珠岩、石膏、改性草木灰和铝粉;粉碎至细度达到180-200目;
(2)搅拌:先加水各自搅拌,然后混合搅拌并按重量份加入原料中的其他剩余原料;
(3)浇注:将步骤(2)搅拌好的浆料加入砖模中,得到砖胚体;
(4)静养:将步骤(3)的砖胚体放入静养室中,静养室密封保温42-48℃,静养时间1-3小时;
(5)切割:将步骤(4)静养好的砖胚体放到切割机上加工成一定所需尺寸;
(6)蒸养:将上述步骤(5)的生坯在0.7-0.9Mpa蒸汽养护17-20h,即得加气砖成品。
改性草木灰是将草木灰研磨成100-200目粉末,拌入相当于粉体重量1-2%的用环氧硬脂酸辛酯、1-2%的木质素磺酸钙拌搅均匀,烘干,粉碎成粉末得到。本发明的有益效果:
本发明通过采用碎玻璃和城市玻璃作为加气砖的成分,有效的减少了环境污染,变废为宝,保护了环境;减少了能源消耗;本发明加气砖隔热与隔音性能均好,较现有加气砖有明显提高;同时本发明通过优化配方用料,本发明的强度、抗冻性有了明显提高。
具体实施方式
实施例1:以碎玻璃为基质的加气砖,其组成原料的重量份为:碎玻璃49-52、城市污泥5-6、水泥5-6、云母粉5-6、膨胀珍珠岩14-16、石膏4-5、改性草木灰4、铝粉0.03-0.05、凹凸棒土0.5-1、平平加0.03-0.04、纯碱0.03-0.05、氢氧化铝0.01-0.02、三乙醇胺0.01-0.02和壳聚糖0.3-0.5。
以碎玻璃为基质的加气砖的加工方法,包括以下步骤:
(1)原材料的处理:原材料包括碎玻璃、城市污泥、水泥、云母粉、膨胀珍珠岩、石膏、改性草木灰和铝粉;粉碎至细度达到180-200目;
(2)搅拌:先加水各自搅拌,然后混合搅拌并按重量份加入原料中的其他剩余原料;
(3)浇注:将步骤(2)搅拌好的浆料加入砖模中,得到砖胚体;
(4)静养:将步骤(3)的砖胚体放入静养室中,静养室密封保温42-48℃,静养时间1-3小时;
(5)切割:将步骤(4)静养好的砖胚体放到切割机上加工成一定所需尺寸;
(6)蒸养:将上述步骤(5)的生坯在0.7-0.9Mpa蒸汽养护17-20h,即得加气砖成品。
改性草木灰是将草木灰研磨成100-200目粉末,拌入相当于粉体重量1.2%的用环氧硬脂酸辛酯、1.2%的木质素磺酸钙拌搅均匀,烘干,粉碎成粉末得到。通过上述实施例1加工得到的加气砖的性能数据如下:孔隙达71%-79%,体积密度610~770kg/m3,耐火温度为715℃,导热系数为0.12-0.18W/MK,吸水导湿缓慢,同体积吸水至饱和所需时间是粘土砖的5.8倍。抗压强度为5.1-7.2Mpa。

Claims (3)

1.一种以碎玻璃为基质的加气砖,其特征在于其组成原料的重量份为:碎玻璃40-55、城市污泥5-10、水泥5-8、云母粉5-10、膨胀珍珠岩14-16、石膏4-5、改性草木灰2-4、铝粉0.03-0.05、凹凸棒土0.5-1、平平加0.03-0.04、纯碱0.03-0.05、氢氧化铝0.01-0.02、三乙醇胺0.01-0.02和壳聚糖0.3-0.5。
2.一种如权利要求1所述的以碎玻璃为基质的加气砖的加工方法,其特征在于包括以下步骤:
(1)原材料的处理:原材料包括碎玻璃、城市污泥、水泥、云母粉、膨胀珍珠岩、石膏、改性草木灰和铝粉;粉碎至细度达到180-200目;
(2)搅拌:先加水各自搅拌,然后混合搅拌并按重量份加入原料中的其他剩余原料;
(3)浇注:将步骤(2)搅拌好的浆料加入砖模中,得到砖坯体;
(4)静养:将步骤(3)的砖坯体放入静养室中,静养室密封保温42-48℃,静养时间1-3小时;
(5)切割:将步骤(4)静养好的砖坯体放到切割机上加工成一定所需尺寸;
(6)蒸养:将上述步骤(5)的生坯在0.7-0.9MPa蒸汽养护17-20h,即得加气砖成品。
3.根据权利要求1所述的以碎玻璃为基质的加气砖,其特征在于:所述的改性草木灰是将草木灰研磨成100-200目粉末,拌入相当于粉体重量1-2%的环氧硬脂酸辛酯、1-2%的木质素磺酸钙拌搅均匀,烘干,粉碎成粉末得到。
CN201210320638.4A 2012-09-03 2012-09-03 一种以碎玻璃为基质的加气砖及其加工方法 Active CN102887672B (zh)