CN102009000A - 一种用于金、银和铂族元素的捕收剂的制备及其使用方法 - Google Patents

一种用于金、银和铂族元素的捕收剂的制备及其使用方法 Download PDF

Info

Publication number
CN102009000A
CN102009000A CN 201010237428 CN201010237428A CN102009000A CN 102009000 A CN102009000 A CN 102009000A CN 201010237428 CN201010237428 CN 201010237428 CN 201010237428 A CN201010237428 A CN 201010237428A CN 102009000 A CN102009000 A CN 102009000A
Authority
CN
China
Prior art keywords
collecting agent
gold
silver
flotation
ore
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN 201010237428
Other languages
English (en)
Other versions
CN102009000B (zh
Inventor
王强
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Beijing Tianrenruichuang Science & Technology Development Co Ltd
Original Assignee
Beijing Tianrenruichuang Science & Technology Development Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Beijing Tianrenruichuang Science & Technology Development Co Ltd filed Critical Beijing Tianrenruichuang Science & Technology Development Co Ltd
Priority to CN201010237428.XA priority Critical patent/CN102009000B/zh
Publication of CN102009000A publication Critical patent/CN102009000A/zh
Application granted granted Critical
Publication of CN102009000B publication Critical patent/CN102009000B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明介绍了一种用于金、银和铂族元素的捕收剂的制备方法,它是采用在烯丙基烷基硫氨酯的黑药溶液中添加烷醇在室温下充分搅拌至透明得到的。本发明还提供了该捕收剂的使用方法,将矿石研磨至适宜的细度,使矿浆中的固体质量含量为20~50%,然后加入石灰或硫酸调整矿浆的pH值在8.0~11.0之间,最后加入4~30g/t起泡剂和2~100g/t捕收剂,按照常规泡沫浮选方法浮选金、银和铂族金属。本捕收剂选择性好,捕收性能高,泡沫粘性适中,大大提高了精矿中金、银、铂/钯金属的品位和回收率。

Description

一种用于金、银和铂族元素的捕收剂的制备及其使用方法
(一)技术领域
本发明涉及一种用于金、银和铂族元素捕收剂的制备及其使用方法。
(二)背景技术
泡沫浮选是技术成熟、分选效率高、应用范围广的矿物加工分选方法,其主要特征是利用矿物表面润湿性差异,在固-液-气三相界面有选择性富集一种或几种目的物料。在泡沫浮选工艺中常用的捕收剂有黄药、黑药、硫氨酯、黄原酸甲酸酯、硫脲等。
美国专利US 3,925,218公开了油溶性的二烷基硫氨酯溶于二烷基二硫代磷酸盐(俗称黑药,下称黑药)水溶液中,制得的混合物溶液有助于改善铜的浮选回收率。可能原因是二烷基硫氨酯溶于黑药水溶液,有助于其在矿浆中的分散,从而提高其捕收性能。
美国专利US 5,232,581公开了油溶性烯丙基烷基硫氨酯溶于黑药水溶液制得的混合物溶液具有协同效应,可以在中性至碱性条件下从贱金属矿石中浮选金、银和铂族金属,回收率也有所改善。
上述的烯丙基烷基硫氨酯溶于黑药制得的浮选金、银和铂族金属的捕收剂也存在缺陷。首先,该捕收剂有起泡性,其泡沫粘性大;其次,因为油状的硫氨酯在黑药的水溶液中溶解度是有限的,需和辅助捕收剂一起使用效果更佳,当辅助捕收剂是硫氨酯时,同样存在在矿浆中快速扩散的问题。
(三)发明内容
本发明的目的是提供一种选择性好、捕收能力高、泡沫粘性适中的复配型浮选捕收剂及其使用方法。本发明采用在烯丙基烷基硫氨酯的黑药溶液中添加烷醇,从而改善捕收剂的泡沫粘度,还能提高硫氨酯在黑药溶液中的溶解度。另外当采用硫氨酯做辅助捕收剂时,可以增加硫氨酯在水溶液中的分散速度,同时降低浮选操作时起泡剂的添加量,提高金、银和铂族金属的回收率,增加经济效益。
本发明为复配型浮选捕收剂,用于回收金、银和铂族金属,由捕收剂黑药、烯丙基烷基硫代氨基甲酸酯和醇组成。其中黑药的分子式如下:
Figure BSA00000205714400011
式子(I)中R为C2-C8的烷基,X为碱金属(如钠、钾等)以及铵。
烯丙基烷基硫氨酯的分子式如下
Figure BSA00000205714400012
式子(II)中R也为C2-C8的烷基。
醇可以是直链烷醇,也可以是支链烷醇,分子式如下:
R-OH    (III)
式子(III)中R为C3-C9的烷基,最好是C4-C7的烷基。
本发明黑药和硫氨酯的体积比为80∶20至20∶80,最好为65∶35至35∶65,而醇占混合物总体积的0.5-5%。
本发明捕收剂制备方法简单,按比例把黑药、硫氨酯与醇加入容器中,在室温下充分搅拌至透明即可。
本发明还提供了该捕收剂的使用方法。首先是磨矿,用球磨机将矿石研磨至适宜的细度,粗、细产品分别为+75μm质量含量在14%到40%之间,-38μm的质量含量在40%到90%之间;接着制备矿浆,使矿浆中的固体质量含量为20~50%;然后是调浆,通过加入石灰调整矿浆的pH值在8.0~11.0之间;最后是浮选,加入起泡剂和上述捕收剂,通常,每吨矿石大约加2~100克的捕收剂,4~30克起泡剂,按照常规泡沫浮选方法浮选金、银和铂族金属。
本发明捕收剂可以单独使用,与辅助捕收剂(如黄药、黑药、硫氨酯、硫脲、巯基苯并噻唑)一起使用效果更好。辅助捕收剂的用量不超过捕收剂总质量的50%。
(四)具体实施方式
本发明由下列实例进一步说明,但不受这些实例的限制。
在容器中加入黑药溶液,然后在搅拌下加入烯丙基烷基硫氨酯,最后加入烷醇,使其混合均匀,即得本发明产品。
用球磨机将矿石研磨到粗、细产品细度分别为+75μm质量含量占40%,-38μm的质量含量占90%,粗粒浮选产出精矿1,粗粒浮选尾矿返回原磨机再磨再选,细粒采用搅拌式浮选机浮选别,一次粗选、一次扫选,三次精选,分别产出精矿2和尾矿。
实例1-5中,选用异丁钠黑药(A)、N-烯丙基-O-乙基硫氨酯(B)、正丁醇制得捕收剂浮选某硫化矿中金,捕收剂用量70g/t,药剂制度见表1。
表1:实例1-5捕收剂的组份及配比
  实施例   A∶B(体积比)   正丁醇(g/t)   精矿2(品位g/t)  精矿1+2(回收率%)
  1   80∶20   2   12.15  86.80
  2   60∶40   2   17.65  94.78
  3   50∶50   2   15.60  90.55
  4   40∶60   2   16.87  92.26
  5   20∶80   2   14.26  89.36
表1可看出,异丁钠黑药(A)、N-烯丙基-O-乙基硫氨酯(B)比例为60∶40-40∶60时,金精矿的品位和回收效果较好。
实例6-10中,异丁钠黑药(A)∶N-烯丙基-O-乙基硫氨酯(B)=60∶40的条件下,改变正丁醇的加入量制得捕收剂浮选某硫化矿中金,捕收剂用量70g/t,药剂制度见表2。
表2:实例6-10捕收剂的组份及配比
  实施例   A∶B(体积比)   正丁醇(g/t)   精矿2(品位g/t)  精矿1+2(回收率%)
  6   60∶40   0   13.55  89.81
  7   60∶40   1   14.68  92.41
  8   60∶40   2   15.76  95.02
  9   60∶40   3   15.62  94.86
  10   60∶40   4   16.87  95.10
表2可看出,随着正丁醇逐量加入,金精矿的品位和回收率逐步提高,当正丁醇用量≥2g/t时,随着用量的增加,品位和回收率增加不明显,考虑到成本,选择正丁醇用量为2g/t。
实例11-15中,选用不同的黑药(A)和硫氨酯(B)进行复配,对几种含金、铂/钯矿石进行浮选,捕收剂用量均为70g/t。与原矿相比品味提高和回收率结果如表3。
表3:实例11-15捕收剂的组份及配比
表3可看出,在浮选金、银、铂金属时,本发明捕收剂在单独使用和与辅助捕收剂协同使用时,精矿品位和回收率都达到了比较好的效果。

Claims (2)

1.一种用于金、银和铂族元素的捕收剂的制备方法,原料为烯丙基烷基硫氨酯、黑药、烷醇,其特征在于:按比例把黑药、硫氨酯与醇加入容器中,在室温下充分搅拌至透明即可,黑药和硫氨酯的体积比为80∶20至20∶80,醇占混合物总体积的0.5-5%;
2.一种针对权利要求1所述捕收剂的使用方法,包括用球磨机将矿石研磨至适宜的细度,+75μm质量含量在14%到40%之间,-38μm的质量含量在40%到90%之间,接着制备矿浆,使矿浆中的固体质量含量为20~50%,然后是调浆,通过加入石灰或硫酸对调整矿浆的pH值使其在8.0~11.0之间,浮选工艺为:矿石研磨到粗、细产品细度分别为+75μm质量含量占40%,-38μm的质量含量占90%,加入起泡剂和上述捕收剂,通常,每吨矿石大约加2~100克的捕收剂,起泡剂为每吨矿石约4~30克左右,按照常规泡沫浮选方法浮选金、银和铂族金属,粗粒浮选产出精矿1,粗粒浮选尾矿返回原磨机再磨再选,细粒采用搅拌式浮选机浮选别,一次粗选、一次扫选,三次精选,分别产出精矿2和尾矿。
CN201010237428.XA 2010-07-27 2010-07-27 一种用于金、银和铂族元素的捕收剂的制备及其使用方法 Active CN102009000B (zh)